Cause analysis and solution of plastic shell dent

Release time:2022-02-28

During the injection molding process, the dents of the plastic shell are shrinkage dents generated after the plastic is cooled and hardened, which mainly appear in the thick wall of the plastic shell, ribs, shell, nut insert back, etc.

3.jpg


1、 Equipment:

(1) Insufficient feeding

The screw or plunger is seriously worn, and the molten material leaks during the injection and pressure maintaining process, which reduces the mold filling pressure and the amount of molten material, resulting in insufficient molten material.


(2) Nozzle hole too large or too small

If it is too small, it is easy to block the sprue; if it is too large, the injection force is small, and it is difficult to fill the mold.


2、 Mold:

(1) The gate is too small or the runner is too narrow or shallow, the runner efficiency is low, the resistance is large, and the molten material is cooled too early.

The gate cannot be too large, otherwise the shear rate will be lost, the material viscosity is high, and the plastic shell will not be full. The gate should be opened on the thick wall of the plastic shell. By setting up a cold charging well with sufficient capacity in the flow channel, the cold charging can be excluded from entering the mold cavity, so that the mold filling can continue.

The gate length of point gate and needle gate must be controlled below 1mm, otherwise the plastic will solidify rapidly in the gate, affecting the pressure transmission; If necessary, increase the number of point gates or gate positions to meet the actual needs; When the flow passage is long and thick, exhaust grooves should be set at the edge of the flow passage to reduce the blocking effect of air on the flow of materials.


(2) Multi gate mold should adjust the filling speed of each gate, and it is best to set up gates symmetrically.


(3) The key parts of the mold should be effectively set with cooling channels to ensure that the cooling of the mold has a good effect on removing or reducing shrinkage cavities.


(4) The whole mold should be free of burrs, have reliable mold closing tightness, and can withstand the filling of high-pressure, high-speed, low viscosity molten materials.


3、 Technical aspects:

(1) Increase the injection pressure, maintain the pressure and prolong the injection time.

For plastic with high fluidity, high pressure will cause flash and collapse, so the material temperature should be appropriately reduced, and the temperature of the front of the barrel and the nozzle should be reduced, so that the volume change of molten material entering the cavity is reduced, and it is easy to cold solidify; For high viscosity plastics, the barrel temperature should be increased to make it easier to fill the mold. When the gate area shrinks, the pressure holding time should be extended.


(2) Increasing the injection speed can easily fill the parts and remove most of the shrinkage.


(3) The thin-walled plastic shell should increase the mold temperature to ensure the smooth flow of materials; The thick wall plastic shell should reduce the mold temperature to accelerate the curing and shaping of the skin.


(4) The cooling residence time of the plastic shell in the mold is prolonged, the production cycle is kept uniform, the back pressure is increased, and a certain buffer pad is reserved at the front end of the screw, which is conducive to reducing the shrinkage phenomenon.


(5) The low precision plastic shell should be taken out of the mold as soon as possible and cooled slowly in air or hot water, so that the shrinkage depression can become smooth without affecting the use.


4、 Raw materials:

The raw material is too soft and easy to flow. The effective way is to add nucleating agent to the plastic to accelerate crystallization.


5、 Plastic shell design:

The design of plastic shell should make the wall thickness uniform and try to avoid the change of wall thickness. For plastics with large shrinkage such as polypropylene, when the thickness changes by more than 50%, it is best to replace the thickened part with ribs.

Copyright: Shenzhen Zhongyuan Plastic Co., Ltd. | mold processing customized manufacturer. If you want to know the processing price of the factory, how much is it, and which is good, please contact us Yue ICP Bei No. 17060480
国精品无码一区二区三区在线蜜臀 | 欧美中国日本裸交一区二区| 无码色偷偷亚洲国内自拍| 99久久国产热无码精品免费| 国产亚洲精品精品综合伦理| 国产久久亚洲精品视频18| 国产女人高潮视频在线观看| 亚洲日本欧美久久久久久| S夜色视频在线精品永久| 国产一区二区在线观看蜜桃| 91久久精品美女高潮不断| 国产精品又粗又硬又大又长| 成a人片在线观看久亚洲| 国产精品久久久久一区二区三区共| 久久国产高清伦理久久一| 亚洲精品无码中在线播放| 产精品无码久久| 美女女同性A片在线观看| 中文字字幕在线乱码| 日本一区二区免费在线电影 | 91精品手机国产在线能| 欧美日韩国产在线一区二区| 色偷偷色噜噜狠狠网站久久| 97影院秋霞午夜在线观看| 久久久大少妇免费高潮特黄| 中文在线观看播放理论片| 最新国语自产精品视频在| 亚洲精品一区二区三区中文字幕| 国产精品成人久久久久久久| 亚洲桃花岛成人av入口| 女白虎炮击喷水在线白虎| 99精品69视频在线观看| 欧美日韩一级片在线播放| 亚洲福利在线看国产精品| 精品毛片熟女一区二区三区| 亚洲GV永久?码天堂网| 2021亚洲A无码在线| 欧美亚日韩在线日本在线| 夜色福利站www国产在线观看| 亚洲五月久自拍区自拍区| 成人免费毛毛片久久影院|